Welcome to Art Clay
Art Clay Gold 22k - Clay Type


Instructions:

Thank you for purchasing ART CLAY GOLD/K22. As this has different characteristic from original ART CLAY SILVER clay type, please read the directions and precautions before use.

INGREDIENTS: 95% of indicated weight is K22 (Gold 91.7%, Silver 8.3 %). After firing: K22 100%

FIRING TEMPERATURE / HOLDING TIME: 1814ºF for 60 min.

MELTING POINT: 1931ºF


[Directions]
Preparation
  • Take out only the necessary amount of clay, wrap it in plastic wrap and knead it well. If it is stiff at first, warm it in your palm a little while. Place the unused portion of clay in a zip loc bag and keep it in an air-tight container at room temperature to prevent it from drying up.
Molding
  • To join Art Clay Gold together or to mend a jointed area, use Art Clay Gold in paste form, which can be made as follows: Put Art Clay Gold in a small plate Add a few drops of water and blend it evenly with something like a spatula.

  • Shape as you wish using your fingers, a mold, etc. If Art Clay Gold becomes stiff to handle, place it in a zip loc bag, add a few drops of water, and knead it until it becomes soft.

Note: Remember that the finished piece shrinks 15%, so size your piece accordingly.

Drying
Condition for Drying

Dry the piece completely at room temperature (more than 24 hours) or by a hair dryer, etc.

Hair
Dryer
Approximately 10-15 minutes with 1200w hair dryer. Place the dryer within 6 inches from the piece.
Cooking
Plate
Approximately 10 min. at 300-350ºF.
Electric Kiln
Approximately 10 minutes 300ºF

Drying time is varies by size of the piece.
  • How to Check If the Piece is Completely Dried
    Place the piece on a flat stainless, glass or plastic plate. After 10~20 seconds remove the piece. If there is no area of condensation left behind, it is completely dried.
Firing
Place the piece in the kiln. (If you are firing more than two pieces, make sure the pieces are not touching each other)

Temperature
1814ºF
Holding Time
60 min.

Take out the piece when the kiln temperature falls below 1112ºF.
Finishing
  • The surface of the fired piece will be matte, but luster can be obtained by polishing. ( e.g. stainless brush, burnisher, sandpaper, etc.)
Completing
  • After firing: K22 - 100%.


[Precautions]

  • Keep the clay Indoors out of direct sunlight.
  • Use it as soon as possible after opening the package.
  • Be careful of hot surfaces.
  • Ventilate your workroom well during firing.
  • Keep this product out of the reach of children.
  • If you get any of this product in your eyes or mouth, flush immediately with plenty of water and call your physician.